基于生物浸提技术的钴白合金中铜和钴的浸出效果及浸出机理

赵伟旭, 田炳阳, 郭献军, 李志华, 苗雅慧, 张世豪, 王佳, 辛宝平. 基于生物浸提技术的钴白合金中铜和钴的浸出效果及浸出机理[J]. 环境工程学报, 2021, 15(5): 1679-1687. doi: 10.12030/j.cjee.202009128
引用本文: 赵伟旭, 田炳阳, 郭献军, 李志华, 苗雅慧, 张世豪, 王佳, 辛宝平. 基于生物浸提技术的钴白合金中铜和钴的浸出效果及浸出机理[J]. 环境工程学报, 2021, 15(5): 1679-1687. doi: 10.12030/j.cjee.202009128
ZHAO Weixu, TIAN Bingyang, GUO Xianjun, LI Zhihua, MIAO Yahui, ZHANG Shihao, WANG Jia, XIN Baoping. Bioleaching process and mechanism of Cu and Co in cobalt white alloy[J]. Chinese Journal of Environmental Engineering, 2021, 15(5): 1679-1687. doi: 10.12030/j.cjee.202009128
Citation: ZHAO Weixu, TIAN Bingyang, GUO Xianjun, LI Zhihua, MIAO Yahui, ZHANG Shihao, WANG Jia, XIN Baoping. Bioleaching process and mechanism of Cu and Co in cobalt white alloy[J]. Chinese Journal of Environmental Engineering, 2021, 15(5): 1679-1687. doi: 10.12030/j.cjee.202009128

基于生物浸提技术的钴白合金中铜和钴的浸出效果及浸出机理

    作者简介: 赵伟旭(1995—),男,硕士研究生。研究方向:涉重危废的生物淋滤资源化处置。E-mail:541776119@qq.com
    通讯作者: 辛宝平(1969—),男,博士,教授。研究方向:涉重危废的生物淋滤资源化处置。E-mail:xinbaoping@bit.edu.cn
  • 中图分类号: X781.18

Bioleaching process and mechanism of Cu and Co in cobalt white alloy

    Corresponding author: XIN Baoping, xinbaoping@bit.edu.cn
  • 摘要: 钴白合金是铜钴矿深加工过程中的副产物,其中的钴、铜等金属资源具有较高的回收价值。利用3种混合菌体系(At、Af、Lf)浸提钴白合金中的铜和钴,考察了在不同固液比下非接触和接触浸提铜和钴的浸出率并对其浸出机理进行了探究。在非接触浸出1%固液比下,钴的浸出率为100%,浸出浓度为1 356.14 mg·L−1,铜的浸出率为77.42%,浸出浓度为837.19 mg·L−1;在该固液比下循环浸出10次,浸出液中铜和钴的质量浓度分别富集到了7 358.67和12 877.25 mg·L−1。在接触浸出4%固液比下,浸出5 d,钴100%浸出,铜基本留存在残渣中。通过对比生物淋滤中的接触浸出和非接触浸出实验的浸出渣中铜和钴的赋存形态可知,钴白合金中钴的浸出机理为生物酸的直接作用,铜的浸出机理为生物酸和Fe3+的共同作用。而在有细菌参与的浸出体系内,存在着铜的浸出消耗导致Fe3+转化成Fe2+和细菌又将Fe2+转化成Fe3+的循环。利用生物浸出循环富集工艺,可高效回收钴白合金中的铜和钴。
  • 加载中
  • 图 1  钴白合金中铜、钴、铁的赋存形态分析

    Figure 1.  Chemical morphology of Cu, Co and Fe of cobalt white alloy

    图 2  钴白合金的XRD图谱

    Figure 2.  XRD patterns of cobalt white alloy

    图 3  钴白合金的SEM图

    Figure 3.  SEM micrographs of cobalt white alloy

    图 4  细菌生长过程中体系的pH、菌数变化

    Figure 4.  Changes in pH and bacterial count of the system during bacterial growth

    图 5  细菌生长过程中体系的Fe3+、Fe2+浓度变化

    Figure 5.  Changes of Fe3+ and Fe2+ concentration in the system during bacterial growth

    图 6  不同固液比下非接触浸出钴白合金中钴铜的浸出率

    Figure 6.  Target metal leaching rate of non-contact bioleaching of cobalt white alloy at different solid-liquid ratios

    图 7  固液比1%下钴白合金浸出渣中铜、钴、铁的赋存形态分析

    Figure 7.  Chemical morphology of Cu, Co and Fe of cobalt white alloy leaching slag under 1% solid-to-liquid ratio

    图 8  固液比1%下非接触不同循环次数下钴白合金中钴铜的浸出浓度

    Figure 8.  Concentration of cobalt white alloy target metal leaching with the number of cycles under 1% solid-to-liquid Ratio

    图 9  不同固液比下接触浸出钴白合金中钴和铜的浸出率

    Figure 9.  Co and Cu leaching rate of contact bioleaching of cobalt white alloy at different solid-liquid ratios

    图 10  接触浸出过程中pH和菌数的变化

    Figure 10.  Changes in pH and bacterial count during contact leaching process

    图 11  接触浸出过程中Fe3+浓度的变化

    Figure 11.  Change of Fe3+ concentration during contact leaching

    图 12  钴白合金淋滤前后的XRD图谱

    Figure 12.  XRD patterns of cobalt white alloy before and after leaching

    图 13  不同固液比下接触浸出第1天残渣中金属赋存形态变化

    Figure 13.  Changes of metal forms in residues on the first day of contact leaching with different solid-to-liquid ratios

    表 1  钴白合金中的金属元素种类及含量

    Table 1.  Types and contents of metal elements in cobalt white alloy %

    CuCoFeNiMnZnAs
    10.8113.6020.530.370.370.080.01
    CuCoFeNiMnZnAs
    10.8113.6020.530.370.370.080.01
    下载: 导出CSV
  • [1] 刘东辉, 钟轩, 熊以俊. ICP-OES法测定钴白合金中主元素含量[J]. 广州化工, 2020, 48(17): 64-67. doi: 10.3969/j.issn.1001-9677.2020.17.023
    [2] 焦翠燕, 郭学益. 钴白合金处理工艺进展及研究方向[J]. 金属材料与冶金工程, 2011, 39(2): 58-63. doi: 10.3969/j.issn.1005-6084.2011.02.014
    [3] 胡宇杰, 孙培梅, 李洪桂, 等. 废硬质合金的回收再生方法及研究进展[J]. 稀有金属与硬质合金, 2004, 53(3): 53-57. doi: 10.3969/j.issn.1004-0536.2004.03.015
    [4] CRUNDWELL F K, DUPREEZ N B, KNIGHTS B D H. Production of cobalt from copper-cobalt ores on the African Copperbelt: An overview[J]. Minerals Engineering, 2020, 156(7): 106450.
    [5] 王含渊, 江培海, 张寅生, 等. 钴白合金湿法冶金工艺研究[J]. 矿冶, 1997, 6(1): 68-70.
    [6] 杜长福, 纪方力. 从钴白合金提取钴铜工业生产概述[J]. 世界有色金属, 2015, 2(11): 107-108.
    [7] REN G, LIU Z, PAN B, et al. A novel process for cobalt and copper recovery from cobalt white alloy with high silicon[J]. Metallurgical Research & Technology, 2020, 117(4): 404.
    [8] YU X, LI Y, LUO Z, et al. Wetting behavior and mechanism of glass coatings on samarium-cobalt alloys in the heating process[J]. Ceramics International, 2020, 46(14): 22980-22986. doi: 10.1016/j.ceramint.2020.06.073
    [9] 徐志峰, 月日辉, 严康, 等. 复杂高硅钴白合金碱焙烧脱硅预处理[J]. 中国有色金属学报, 2012, 22(10): 2916-2923.
    [10] 刘卓君, 刘欣, 李林艳, 等. 钴白合金的常压浸出工艺研究[J]. 有色金属科学与工程, 2015, 6(1): 24-28.
    [11] 曹洪杨, 金明亚, 王继民, 等. 氧压酸浸在含锗铜钴白合金有价组分分离中的应用[J]. 材料研究与应用, 2016, 10(2): 131-134. doi: 10.3969/j.issn.1673-9981.2016.02.013
    [12] 熊以俊, 刘东辉. 机械活化强化钴白合金酸浸钴的试验研究[J]. 湿法冶金, 2015, 34(4): 292-295.
    [13] 洪侃, 范进军, 卢博, 等. 铜钴合金双膜电化学溶解造液造碱研究[J]. 江西理工大学学报, 2010, 31(2): 17-20.
    [14] 胡国宏. 氧化亚铁硫杆菌浸出钴白合金研究[D]. 长沙: 中南大学, 2012.
    [15] 胡国宏, 肖利, 方正, 等. 氧化亚铁硫杆菌浸出钴白合金[J]. 过程工程学报, 2012, 12(2): 200-205.
    [16] 牛志睿, 江明荣, 李倩, 等. 超声辅助生物淋滤废旧Zn-C电池锌锰溶出的研究[J]. 环境科学学报, 2016, 36(9): 3313-3321.
    [17] TORMA A E. Biotechnology applied to mining of metals[J]. Biotechnol Adv, 1983, 1(1): 73-80.
    [18] 王畅,杜虹,杨运云,等. 重金属形态连续萃取法对沉积物矿物相态的影响[J]. 分析化学, 2011, 39(12): 1887-1892.
    [19] 王畅,夏冰,王冠华,等. 缺氧沉积物中重金属形态连续萃取方法的稳定性研究[J]. 分析测试学报, 2012, 31(4): 470-474.
    [20] 揭诗琪, 邵继莹, 吴雨桐, 等. 生物淋滤结合类芬顿反应去除底泥中重金属[J]. 有色金属科学与工程, 2016, 7(1): 108-113.
    [21] 张祥楠. 生物淋滤法去除污泥中重金属[D]. 沈阳: 沈阳建筑大学, 2012.
    [22] 杨洁, 蔡体久, 汪群慧, 等. 直接与间接生物淋滤法去除城市生活垃圾焚烧飞灰中重金属的研究[J]. 北京林业大学学报, 2008, 30(S1): 267-271.
    [23] 辛宝平, 李是珅, 赵小鹭, 等. 废旧锂离子电池中钴的生物淋滤机制[J]. 科学通报, 2008, 53(23): 2881-2887. doi: 10.3321/j.issn:0023-074X.2008.23.008
    [24] WU H Y, TING Y P. Metal extraction from municipal solid waste (MSW) incinerator fly ash: Chemical leaching and fungal bioleaching[J]. Enzyme and Microbial Technology, 2006, 38(6): 839-847. doi: 10.1016/j.enzmictec.2005.08.012
    [25] RAWLINGS D E, TRIBUTSCH H, HANSFORD G S. Reasons why 'Leptospirillum'-like species rather than Thiobacillus ferrooxidans are the dominant iron-oxidizing bacteria in many commercial processes for the biooxidation of pyrite and related ores[J]. Microbiology, 1999, 145: 5-13. doi: 10.1099/13500872-145-1-5
    [26] 孙艳, 吴锋, 辛宝平, 等. 硫杆菌浸出废旧MH/Ni电池中重金属研究[J]. 生态环境, 2007, 16(6): 1674-1678.
    [27] 黄峰源. 嗜酸性硫杆菌生长特性与耐受重金属机制及污泥淋滤过程中微生物分子生态的研究[D]. 南京: 南京农业大学, 2006.
    [28] 沈镭, 张再利, 贾晓珊. 氧化亚铁硫杆菌和氧化硫硫杆菌对硫代硫酸钠的代谢机理研究[J]. 环境科学学报, 2006, 26(12): 2000-2007. doi: 10.3321/j.issn:0253-2468.2006.12.011
    [29] 陈亮, 代云. 两矿法浸出钴白合金工艺及机制研究[J]. 湿法冶金, 2017, 36(1): 24-27.
    [30] 陈亮. 钴白合金和水钴矿联合高压酸浸的工艺研究[J]. 中国有色冶金, 2016, 45(4): 75-78. doi: 10.3969/j.issn.1672-6103.2016.04.020
    [31] GU T, RASTEGAR S O, MOUSAVI S M, et al. Advances in bioleaching for recovery of metals and bioremediation of fuel ash and sewage sludge[J]. Bioresource Technology, 2018, 261: 428-440. doi: 10.1016/j.biortech.2018.04.033
    [32] NARESHKUMAR R, NAGENDRAN R. Changes in nutrient profile of soil subjected to bioleaching for removal of heavy metals using Acidithiobacillus thiooxidans[J]. Journal of Hazardous Materials, 2008, 156(1-3): 102-107. doi: 10.1016/j.jhazmat.2007.12.001
    [33] DELVASTO P, VALVERDE A, BALLESTER A, et al. Diversity and activity of phosphate bioleaching bacteria from a high-phosphorus iron ore[J]. Hydrometallurgy, 2008, 92(3/4): 124-129. doi: 10.1016/j.hydromet.2008.02.007
    [34] XIA L X, LIU J S, XIAO L, et al. Single and cooperative bioleaching of sphalerite by two kinds of bacteria: Acidithiobacillus ferriooxidans and Acidithiobacillus thiooxidans[J]. Transactions of Nonferrous Metals Society of China, 2008, 18(1): 190-195.
    [35] BURZYMNSKA L, GUMOWSKA W, RUDNIK E, et al. Mechanism of the anodic dissolution of Cu70-Co4-Fe14-Pb7 alloy originated from reduced copper converter slag in an ammoniacal solution[J]. Hydrometallurgy, 2008, 92(1/2): 34-41. doi: 10.1016/j.hydromet.2008.01.009
    [36] FENG R, XU S, LIU J, et al. The influence of Cl on the electrochemical dissolution of cobalt white alloy containing high silicon in a sulfuric acid solution[J]. Hydrometallurgy, 2014, 142: 12-22. doi: 10.1016/j.hydromet.2013.10.006
    [37] KAKSONEN A H, SARKIJARVI S, PEURANIEMI E, et al. Metal biorecovery in acid solutions from a copper smelter slag[J]. Hydrometallurgy, 2017, 168: 135-140. doi: 10.1016/j.hydromet.2016.08.014
  • 加载中
图( 13) 表( 1)
计量
  • 文章访问数:  4823
  • HTML全文浏览数:  4823
  • PDF下载数:  59
  • 施引文献:  0
出版历程
  • 收稿日期:  2020-09-17
  • 录用日期:  2020-10-15
  • 刊出日期:  2021-05-10
赵伟旭, 田炳阳, 郭献军, 李志华, 苗雅慧, 张世豪, 王佳, 辛宝平. 基于生物浸提技术的钴白合金中铜和钴的浸出效果及浸出机理[J]. 环境工程学报, 2021, 15(5): 1679-1687. doi: 10.12030/j.cjee.202009128
引用本文: 赵伟旭, 田炳阳, 郭献军, 李志华, 苗雅慧, 张世豪, 王佳, 辛宝平. 基于生物浸提技术的钴白合金中铜和钴的浸出效果及浸出机理[J]. 环境工程学报, 2021, 15(5): 1679-1687. doi: 10.12030/j.cjee.202009128
ZHAO Weixu, TIAN Bingyang, GUO Xianjun, LI Zhihua, MIAO Yahui, ZHANG Shihao, WANG Jia, XIN Baoping. Bioleaching process and mechanism of Cu and Co in cobalt white alloy[J]. Chinese Journal of Environmental Engineering, 2021, 15(5): 1679-1687. doi: 10.12030/j.cjee.202009128
Citation: ZHAO Weixu, TIAN Bingyang, GUO Xianjun, LI Zhihua, MIAO Yahui, ZHANG Shihao, WANG Jia, XIN Baoping. Bioleaching process and mechanism of Cu and Co in cobalt white alloy[J]. Chinese Journal of Environmental Engineering, 2021, 15(5): 1679-1687. doi: 10.12030/j.cjee.202009128

基于生物浸提技术的钴白合金中铜和钴的浸出效果及浸出机理

    通讯作者: 辛宝平(1969—),男,博士,教授。研究方向:涉重危废的生物淋滤资源化处置。E-mail:xinbaoping@bit.edu.cn
    作者简介: 赵伟旭(1995—),男,硕士研究生。研究方向:涉重危废的生物淋滤资源化处置。E-mail:541776119@qq.com
  • 1. 烟台大学环境与材料工程学院,烟台 264005
  • 2. 北京理工大学材料学院,北京 100081

摘要: 钴白合金是铜钴矿深加工过程中的副产物,其中的钴、铜等金属资源具有较高的回收价值。利用3种混合菌体系(At、Af、Lf)浸提钴白合金中的铜和钴,考察了在不同固液比下非接触和接触浸提铜和钴的浸出率并对其浸出机理进行了探究。在非接触浸出1%固液比下,钴的浸出率为100%,浸出浓度为1 356.14 mg·L−1,铜的浸出率为77.42%,浸出浓度为837.19 mg·L−1;在该固液比下循环浸出10次,浸出液中铜和钴的质量浓度分别富集到了7 358.67和12 877.25 mg·L−1。在接触浸出4%固液比下,浸出5 d,钴100%浸出,铜基本留存在残渣中。通过对比生物淋滤中的接触浸出和非接触浸出实验的浸出渣中铜和钴的赋存形态可知,钴白合金中钴的浸出机理为生物酸的直接作用,铜的浸出机理为生物酸和Fe3+的共同作用。而在有细菌参与的浸出体系内,存在着铜的浸出消耗导致Fe3+转化成Fe2+和细菌又将Fe2+转化成Fe3+的循环。利用生物浸出循环富集工艺,可高效回收钴白合金中的铜和钴。

English Abstract

  • 钴白合金是铜钴矿深加工过程中的副产物,由于钴的存在,使得该合金具有良好的硬度及耐热性[1]。钴白合金的成分基本为钴、铜、铁,其他元素的含量极低[2]。我国可利用的钴矿石资源较少,大部分钴矿石依赖进口[3]。世界上最主要的钴资源是刚果(金)和赞比亚的铜钴矿,一般含钴品位为0.1%~0.5%,高品味的可达到2%~3%。但是,其副产物钴白合金中钴的含量可达10%左右;此外,在钴白合金中,还含有大量的铜、铁等元素,使其具有较高的回收价值[1-5]

    目前,钴白合金的回收处理工艺主要有火法、湿法和微生物浸出等[6]。火法处理的常规工艺为造渣熔炼-浸出工艺[7]。该工艺先通过向钴白合金中掺入碳酸钙等配料,之后再在高温下焙烧,以实现钴、铜与其他杂质金属的分离,最终通过硫酸酸浸得到钴和铜的浸出液。但是,火法处理的能耗较高,操作也相对复杂,而且对有价金属的回收不彻底[8-9]。湿法处理主要有常压氧化酸浸法[10]、加压氧化酸浸法[11]、机械活化-酸浸法[12]、电化学溶解法[13]。相比于火法处理,湿法处理能耗低,但是对于处理设备的要求较高,同时也会产生一定的环境污染。有研究结果表明,使用微生物浸出钴白合金可实现钴、铜的高效回收[14]。胡国宏等[15]使用A.f菌(氧化亚铁硫杆菌)进行钴白合金的浸出,钴和铜的浸出率分别可以达到了99.5%和99.0%,而且浸出率高、成本低。

    本研究通过消解分析钴白合金中各种金属的含量,初步估计其资源化利用的价值;并通过梯度实验探究接触浸出和非接触浸出的最佳固液比,以选出最佳工艺的最佳处理条件;最终,通过接触浸出和非接触浸出实验结果的对比分析,探究这2种方法对钴白合金中钴和铜的浸出机理。

  • 供试钴白合金来源于河南某有色冶炼厂。盐酸(HCl)、硝酸(HNO3)、高氯酸 (HClO4)、氢氟酸(HF)、硫磺(S)、黄铁矿(FeS2)、硫酸铵((NH4)2SO4)、磷酸二氢钾 (KH2PO4)、无水氯化钙 (CaCl2)、七水合硫酸镁(MgSO4·7H2O)、醋酸(HOAc)、盐酸羟胺(NH2OH·HCl)、双氧水(H2O2)、醋酸铵(NH4OAc)均为分析纯。

  • 电感耦合等离子发射光谱仪(OPTIMA 8300,珀金埃尔默股份有限公司)用于测定溶液中金属元素的浓度;X射线衍射仪(VG MK II,英国VG公司)用于分析固体样品的晶体结构;扫描电子显微镜SEM(Quanta FEG 250,美国FEI公司)用于观察固体样品的微观形貌;电热恒温鼓风干燥箱(DHP-9032,上海一恒科学仪器有限公司);pH计(DELTA320,梅特勒-托利多仪器有限公司);恒温水浴振荡器(THZ-82,金坛市荣华仪器制造有限公司)用于培养混合菌液。

  • 将钴白合金置于电热恒温鼓风干燥箱中105 ℃烘干至恒重,粉碎研磨,过100目筛筛分后备用。钴白合金的金属含量测定采用三酸消解法[1, 16],目标金属的赋存形态采用BCR连续萃取法[17-19]

  • 取若干容积为250 mL的锥形瓶,先分别加入85 mL无机盐培养基[20-23](2.0 g·L−1 (NH4)2SO4、1.0 g·L−1 KH2PO4、0.25 g·L−1 CaCl2、0.5 g·L−1 MgSO4·7H2O)、0.8 g硫磺、0.8 g黄铁矿;之后,接入At、Af、Lf菌液[24-25]各5 mL;透气膜封口后,置于恒温水浴振荡器中,在35 ℃条件下,以135 r·min−1振荡,培养至体系pH下降至0.8,便可用于生物淋滤实验。

  • 将培养稳定的菌液高速离心后,使菌体和生物酸分离。向pH为0.8的生物酸中直接加入钴白合金样品,并置于恒温水浴振荡器中,在35 ℃、135 r·min−1的条件下反应24 h,此为非接触淋滤实验[26-28]。该浸出过程无细菌参与。设定淋滤的固液比(g∶mL)为1∶100、2∶100、3∶100、4∶100、5∶100、6∶100,每个梯度做3个平行实验。反应结束后,测定上清液中目标金属浓度。

    按照上述最优淋滤效果对应的固液比,做非接触循环富集实验。浸出完成后,通过抽滤实现固液分离;向上清液中加入之前分离出的菌体,密封;之后,于恒温水浴震荡器中,培养条为35 ℃、135 r·min−1,培养至体系pH下降至0.8;再进行非接触淋滤实验。如此循环淋滤10次,之后测定每次淋滤后上清液中的目标金属浓度。

  • 向pH已达到0.8的菌液中直接加入钴白合金,置于恒温水浴震荡器中,在35 ℃、135 r·min−1条件下培养,隔天取样测钴、铜的浸出浓度,此为接触淋滤[26-28]。在该过程中,生物酸和细菌同时参与浸出。设定淋滤的固液比(g∶mL)为1∶100、2∶100、3∶100、4∶100。每个梯度做3个平行实验。在反应的第1、3、5、7、9 d取上清液测定目标金属浓度。

  • 钴白合金样品中的金属种类及含量如表1中所示。其中,钴百合金中含铜量为10.81%、钴为13.66%、铁为20.53%,即有一定的回收价值。但该样品中铁含量过高,在浸出过程中会产生铁钒沉淀,会影响铜、钴的浸出效果。因此,为设计出更加合理的浸出工艺参数,使用BCR连续萃取技术处理钴白合金,以分析其中钴、铜、铁的金属赋存形态[18],所得结果如图1所示。如图1所示,钴白合金中的钴、铜、铁均不存在硫化物及有机结合态。其中,钴的存在形态为酸溶态(46.27%)和氧化物结合态(53.73%);铜的存在形态为酸溶态(7.86%)、氧化物结合态(78.84%)、残渣态(13.3%);铁的存在形态全部为酸溶态。通过BCR实验结果可知,在生物淋滤过程中,样品中的钴通过生物酸中氢离子的作用,基本上可以被完全浸出;铜的浸出除了生物酸的作用外,还需要一定的氧化反应,并可通过菌体的接触实现残渣态铜的浸出。

  • 钴白合金样品的XRD谱图如图2所示。从图中可以看出,钴白合金在43°和45°有2个非常明显的峰值。通过与标准图谱卡片PDF#50-0795和PDF#85-1326[29]对比可知,钴白合金中所含的晶体成分主要为钴铁的合金态Co7Fe3和单质铜Cu。

    通过SEM能够直接观察钴白合金的形貌特征、颗粒尺寸,由图3可知,钴白合金的形状均为不规则的球体和长方体,粒度较小,分布均匀[30]

  • 采用At、Af、Lf这3种菌株的混合培养体系,在35 ℃下连续培养,菌体数量在培养至11 d时增长至3.42×108 个·mL−1,菌液的pH从2.0降至0.8(图4)。这是因为,At菌将能源底物中的硫磺转化成了硫酸和供自身生长所需的能量[31]。直接向该菌液中加入钴白合金为接触浸出,该过程具有生物酸和菌体的共同作用;将菌液中的菌体通过高速离心去除,留下pH为0.8的生物酸浸出钴白合金为非接触浸出,该过程无菌体作用。

    图5中可以看出,随着培养时间的延长,菌液中的Fe3+质量浓度不断升高,Fe2+质量浓度极少。这是因为,Af、Lf氧化分解黄铁矿获取能量生长的过程中,伴随着氧化生成了Fe3+;同时,黄铁矿中分解出的硫被At菌转化成硫酸而进入体系中[32-34]

    经非接触浸出1 d后,测得不同固液比下目标金属铜和钴的浸出率如图6所示。随着固液比的升高,钴和铜的浸出率均逐渐下降。从非接触浸出钴白合金的实验中可以看出,最优固液比为1%,在pH为0.8的生物酸下,钴白合金中的酸溶态和氧化物结合态的钴能够100%浸出,其浸出液质量浓度为1 356.14 mg·L−1;而铜的浸出率为77.42%,浸出液质量浓度为837.19 mg·L−1

    将1%固液比下的浸出渣多次水洗后,分析浸出渣中铜、钴、铁的赋存形态。由图7可以看出,浸出渣中未检测出钴;残留的铜中含有48.84%的氧化物结合态和51.15%的残渣态;铁被浸出后,又生成了铁钒沉淀进入了残渣态。因此,在浸出过程中,可先将样品中的钴优先浸出到溶液中;将铜留存在渣相中,富集后再次浸出,以实现钴白合金浸出过程中的铜、钴分离。

    固液比1%下非接触循环第1次到第10次溶液中,铜和钴的质量浓度如图8所示。由图8可知,在循环的过程中,溶液中铜和钴的质量浓度基本呈倍数上升;而且,在实验过程中可以观察到,溶液的颜色有着明显的加深。循环到第10次时,溶液中钴的质量浓度可达12 877.25 mg·L−1,铜的质量浓度可达7 358.67 mg·L−1

  • 不同固液比下,接触浸出钴白合金中钴和铜的浸出率如图9所示。从不同固液比的接触浸出实验中可以看出,钴白合金中钴的浸出效果要明显优于铜的浸出效果。在接触浸出1 d,随着固液比的升高,铜和钴的浸出率逐渐下降。但浸出7 d,在固液比3%下的接触浸出过程中,钴白合金中的钴和铜依然能够完全浸出。

    在非接触浸出实验中,在固液比1%下,仅生物酸作用,浸出反应1 d,钴100%浸出,铜浸出77.42%。这一结果与接触浸出实验中,在生物酸和细菌的双重作用下,浸出反应1 d的浸出效果基本一直。由于钴白合金的加入,抑制了菌体的生长,菌体数量降至2.41×108个·mL−1。但随着浸出时间的延长,菌体逐渐适应了周围的浸出环境,菌体逐渐生长,在浸出5 d时生长到了3.26×108个·mL−1,基本与接触浸出前的菌数一致(图10(b)),从而代谢出了新的生物酸(图10(a))。从图11接触浸出过程中Fe3+的浓度变化可以看出,随着浸出时间的延长,在固液比1%下,浸出3 d,Fe3+的质量浓度降到最低403.67 mg·L−1,铜达到100%浸出。3 d后,Fe3+的浓度逐渐上升。这是因为,铜的浸出需要Fe3+的参与;同时,在Af和Lf的作用下,将生成的Fe2+氧化生成Fe3+[35]。因此,提高接触浸出的固液比,并在足够的额浸出时间下,当铜的浸出所消耗Fe3+的速度与细菌氧化Fe2+成Fe3+的速度一致时,即浸出完全。

  • 通过对比接触浸出和非接触浸出钴白合金的结果,并结合钴白合金中的金属赋存形态以及钴白合金淋滤前后的XRD图谱变化,可以推测出钴白合金中铜和钴的浸出机理。图12为钴白合金淋滤前后的XRD对比图,可见,淋滤前钴白合金XRD衍射图谱中有较为明显的吸收峰;淋滤后钴白合金XRD衍射图谱中几乎没有吸收峰,这表明钴铁合金和单质铜的结构被破坏[14]。此外,经生物淋滤处理后的钴白合金的硬度有着明显的下降,表面也更加疏松,均表明其结构发生了改变。

    在接触浸出1 d后,对不同固液比下的浸出渣中的钴、铜做金属赋存形态(图13)进行了对比分析。由图13(a)可知,随着固液比的升高,钴的浸出率逐渐降低,浸出渣中残余的钴也越来越多。经与原样中钴的对比可以看出,酸溶态的钴被优先浸出到溶液中,而浸出渣中残留的钴均为氧化物结合态。随着浸出时间的延长,体系内的细菌逐渐适应了周围的生存环境,持续代谢出新的生物酸,从而将浸出渣中的钴浸出到溶液中[36]

    同样,由图13(b)可知,随着固液比的升高,铜的浸出率也在逐渐降低。与原样对比,酸溶态的铜也被率先浸出到溶液中,浸出渣中剩余的铜为氧化物结合态和残渣态,该形态的浸出需要Fe3+的参与,最终生成Cu2+和Fe2+进入溶液中[37]。而随着浸出时间的延长,溶液中的Fe2+被细菌又逐渐氧化成Fe3+,Fe3+继续与固相中的铜发生反应,直至Fe3+的生成速率大于其反应的消耗速率时,整个铜的浸出反应达到完全。

  • 1)钴白合金中所含有价金属主要为铜、钴和铁,而且含量均很高(均在10%以上),资源化利用潜力巨大。铜和钴大部分以酸溶态和氧化物结合态存在,适宜于生物淋滤处理。

    2)非接触浸出钴白合金的最适固液比为1%,此时钴可100%浸出,铜浸出率为77.42%。非接触循环富集进行10次,最终浸出液中钴的质量浓度可达12 877.25 mg·L−1、铜的质量浓度可达7 358.67 mg·L−1

    3)钴白合金在接触浸出中,随着浸出时间的延长,铜和钴最终均能完全浸出。从浸出渣中钴和铜的赋存形态可以看出,钴浸出仅需生物酸的作用,铜的浸出除了需生物酸作用,还需Fe3+的参与。在菌体的直接作用下,浸出体系内部形成了Fe3+的生成和消耗的循环,以供给铜浸出。